Row of 12-point head bolts with wide washers on a rusted steel flange, a 12-point socket lying beside them and plant piping behind

A286 12-Point Flange Bolts for Restricted-Access Turbine Connections

Power & Turbines · 12-Point Flange Bolts · Tool Fit, Class & Expansion

Short answer:

A286 12-point flange bolts are used on turbine casings, frames and manifolds where the bolts sit in deep pockets or close rows and a hex head leaves no room for the tool. A 12-point head is smaller across the flats than a hex head of the same thread size, it is driven by a thin-wall 12-point socket, and that socket re-engages every 30 degrees instead of every 60, which matters when the wrench can only swing a short way. The flange under the head works as a built-in washer, so no loose washer has to be placed in a pocket nobody can see into.

Many installation problems on these joints come from tool fit rather than bolt strength: a socket that doesn't fit the pocket, a wrench with no room to swing, or a hex bolt substituted for a 12-point one. So the order has to describe the pocket and the tool, not just the thread size: socket outside diameter and length, swing space, pocket diameter and depth, and the flange diameter at each position.

The material side is ASTM A453 Grade 660 (UNS S66286). Classes A, B and C all have a 130 ksi (895 MPa) minimum tensile strength and an 85 ksi (585 MPa) minimum yield; Class D raises yield to 105 ksi (725 MPa) up to 2-1/2 in. The classes differ in heat treatment, so the drawing's class should go on the order. The 704°C (1300°F) figure on most A286 datasheets is a short-time limit; for long-term load, A286 is usually kept to around 540°C, and above 427°C (800°F) A453 calls for stress-rupture testing.

Expansion is the other check. A286 grows noticeably more than a ferritic steel casing, so on a Cr-Mo flange it sheds preload as it heats; on an austenitic casing the match is much closer. Where the load or temperature is too much for A286, aged Inconel 718 is the usual step up.

BYBOLT makes A286 12-point flange bolts to drawing from 100 pieces, with EN 10204 3.1 certificates.

In this guide

On a restricted-access turbine joint, the hard part is getting a socket onto every bolt, turning it through a useful angle and reaching the same preload at each position. That is why these joints are designed around a 12-point head in the first place, and why a replacement order that only gives the thread size so often goes wrong.

Top-view diagram of an A286 12-point flange bolt in a tight pocket showing socket outside diameter, swing-space arc and pocket size, with the expansion differential and ASTM A453 Grade 660 class minimums
View full-size diagram
Figure: A286 12-point flange bolt in a tight pocket: socket outside diameter, swing-space arc, pocket diameter and depth, with the expansion differential and the A453 Grade 660 class minimums.

Why a 12-point head, and what it asks of the tool

For the same thread size, a 12-point (double-hexagon) head is smaller across the flats than a hex head, so bolts can sit closer together and the socket that drives them can be slimmer. A 12-point socket can also be re-seated every 30 degrees, against 60 for a hex, so a short wrench swing still makes progress. The contact angle on each point is less favourable than a 6-point socket on a hex, which is why 12-point heads are made taller and designed for that drive.

The catch is that the head only works with the right tool. It needs a 12-point socket of the correct size; a 6-point socket won't go on, and an open-end wrench that bears on two corners will damage it. In a deep pocket, socket length matters as much as socket size, and the socket wall has to clear the pocket at full depth.

For each position, the enquiry should give:

  • socket type, outside diameter and length
  • swing space: the angle a wrench handle can travel before it hits the casing, a pipe or the next bolt. Even with 30-degree re-engagement, a pocket that allows only 15 degrees of swing calls for a ratchet, a crowfoot or a different tightening method.
  • pocket diameter and depth, and the distance to the nearest obstruction and to the next bolt head

Metric 12-point flange screws are dimensioned to ASME B18.2.5M, which covers the head, the flange and the width across flats. Inch-series double-hexagon bolts in turbines usually follow the OEM drawing or an aerospace standard. Either way, the flange should be dimensioned separately from the head on the drawing: flange diameter, width across flats and head height. The A286 12-point flange bolt page lists the sizes and standards we make to.

The flange is a washer and a clearance dimension

The flange under the head spreads the clamp load over a larger bearing area than the head alone could. That makes its diameter a clearance dimension as well as a load dimension. It has to fit the pocket, clear the neighbouring heads and sit fully on the clamped face. A flange that overhangs the face or touches the next head won't seat flat, and a bolt that doesn't seat flat won't hold its preload, whatever its class.

Say whether the flange face is plain or serrated, and what surface it bears on. A flange pressing into a soft or scaled face beds in during the first heat-ups and loses clamp load without the bolt turning, so the tightening calculation should be based on the actual surface. Most turbine drawings specify a plain flange on a machined face; serrations are rarely wanted on a joint that is opened at every overhaul.

A286 classes, temperature and expansion

A286 (UNS S66286) bolting is usually bought to ASTM A453 Grade 660. The class matters more than buyers often expect:

A453 Grade 660 class Minimum tensile Minimum yield Note
A, B and C 130 ksi (895 MPa) 85 ksi (585 MPa) Same minimums, different solution and ageing treatments
D (≤ 2-1/2 in) 130 ksi (895 MPa) 105 ksi (725 MPa) Higher yield

Rolled Alloys' A-286 datasheet lists Class A as solution annealed at 1650°F (about 900°C) and Class B at 1800°F (about 980°C), both followed by a 16-hour age at 1300–1400°F. The higher solution temperature is generally chosen for better stress-rupture life, so the class on the OEM drawing should go on the order rather than being left to the supplier. Our note on A286 heat treatment covers what the certificate should show.

Temperature needs the same care. Most datasheets describe A286 as strong up to 704°C (1300°F), but Rolled Alloys qualifies that as short-time strength and gives about 540°C (1000°F) for long-time service. Their typical 1,000-hour rupture strengths are 88 ksi at 538°C and 46 ksi at 649°C, which shows how quickly the margin goes. A453 itself requires stress-rupture testing for design temperatures above 427°C (800°F), and material that hasn't been tested is stamped NR. Bolts for hot positions should be ordered with the stress-rupture test. For more on how strength falls with temperature, see A286 yield strength at temperature.

Expansion is the last check. A286's mean coefficient rises from about 16.5 µm/m·K near room temperature to about 17.3 µm/m·K at 427°C, against roughly 13 µm/m·K for a Cr-Mo steel flange. Over a 100 mm grip and a 300°C rise, A286 grows about 0.12 mm more than the flange, which is a large share of the stretch that holds the preload. On a ferritic casing, then, an A286 bolt loosens as it heats unless the tightening plan allows for it. On an austenitic stainless casing the expansion is much closer.

When to step up to 718, and what not to substitute

Inconel 718 (UNS N07718), bar to ASTM B637 or AMS 5663 (solution treated and aged), AMS 5662 bar aged after machining, or bolting to ASTM A1014, is the usual step up where the load or temperature is beyond A286. Aged 718 has a minimum yield of 150 ksi (1,035 MPa), and its expansion is close to that of a steel casing, so it holds preload better on a ferritic flange. It is also harder to machine and costs more, so it is worth the change only where A286 runs out. The A286 vs 718 comparison goes through the trade-off.

The substitution to watch for runs the other way. A 316 bolt to ASTM A193 B8M fits the same head and socket, but Class 1 B8M has about a third of A286's yield, and the cold-work strength of Class 2 fades in hot service. If a 12-point head can't be sourced in time, push for the correct part rather than fitting a same-size bolt in a weaker alloy or a hex head without tool clearance.

Candidate Specification Where it fits a restricted-access turbine joint What to watch
A286 S66286, ASTM A453 Grade 660 Most 12-point casing and frame bolts Class on the order; stress-rupture test above 427°C; expansion on ferritic casings
Inconel 718 N07718, ASTM B637 / AMS 5663 aged, or AMS 5662 aged after machining Higher load or temperature Aged condition stated and proved on the certificate
316 S31600, ASTM A193 B8M Not a turbine substitute Class 1 is far weaker; Class 2 loses its strength hot

Tightening, lubricant and the set that arrives

State the tightening method for each position: torque, torque-angle or tensioning. Torque-angle, where the nut or bolt is turned a set angle after a snug torque, gives a more repeatable stretch than torque alone where friction varies, but it needs swing space that a tight pocket may not have. Give the preload target the torque was calculated for, and the lubricant, because a torque figure only means a preload under a stated friction condition. A286 threads can gall against A286 or nickel-alloy nuts and inserts, so use the OEM's approved compound and keep lead and sulfur out of it at turbine temperatures.

At an overhaul, look at the removed bolts by position: head rounding, socket marks, flange imprint, and any bolt that had to be cut out. Rounding at one position means the socket, the swing or the pocket is wrong there. Rounding everywhere means the head or the tool is wrong for the joint.

Each delivered set should trace to its heat, class and ageing record, and come with a hardness report on the finished bolts, EN 10204 3.1 certificates, a dimensional report and PMI where the project calls for it.

Lock before ordering Why it matters Document to ask for
Head type, flange diameter, width across flats, head height A flange too large for its pocket won't seat flat Drawing with head and flange dimensioned per position
Socket, swing space, pocket size per position A socket that fits the head but not the pocket can't be used Tool list and pocket drawing
A453 class and stress-rupture test Classes differ in heat treatment; hot bolts need the test Certificate stating class, ageing record, test report
Tightening method, lubricant, mating thread Torque without a friction condition doesn't prove preload Tightening procedure, approved compound
Set list A mixed set can't be traced after a failure Set list by position, 3.1 certificates

Requesting a quote

Send the pocket along with the size. A note such as "M12 A286 12-point flange bolts for a turbine casing joint, ASTM A453 Grade 660 class per OEM drawing, about 15 degrees of swing, pocket diameter and depth from the drawing" lets the engineering team check head, flange, socket clearance and class before quoting. If you're replacing a set that rounded, a photo of a removed bolt shows whether the problem was the tool, the pocket or the head.

The team will confirm class, pocket and tooling with you, then quote A286 12-point flange bolts, with A286 heavy hex nuts where the joint uses through-bolts. Fastener orders start at 100 pieces. For other turbine bolting, see power generation and turbines.

Related specification guides

For an A453 Grade 660 bolting enquiry, define the class, final condition and acceptance requirements. Compare ASTM A453 Grade 660 Classes A–D