45 matching materials

Nickel AlloysUNS N07718View material details
Nickel AlloysUNS N06625View material details
Nickel AlloysUNS N10276View material details

Scroll horizontally to compare all columns.

Compare Materials: Alloy 718, Alloy 625, Alloy C-276
MaterialAlloy 718N07718Alloy 625N06625Alloy C-276N10276

Summary

Material familyNickel AlloysNickel AlloysNickel Alloys
Grade / UNSN07718N06625N10276
SummaryAn age-hardenable nickel alloy for fasteners and components requiring strength and corrosion resistance.A solid-solution-strengthened nickel alloy used in marine and chemical-processing equipment.A nickel-chromium-molybdenum alloy used in corrosive chemical environments.

Performance overview

Material focusStrength developed through agingStrength without an aging treatmentResistance in aggressive chemical media
Physical reference
Density
8.19 g/cm³
Melting range
1260–1336 °C
Supplied technical reference · Scanned PDF page 12 · printed page 24
Density
8.44 g/cm³
Melting range
1290–1350 °C
Supplied technical reference · Scanned PDF page 12 · printed page 24
Density
8.89 g/cm³
Melting range
1325–1370 °C
Supplied technical reference · Scanned PDF page 11 · printed page 23
Chemical composition
Chemical composition

Composition limits · wt.%

Ni
50–55
Cr
17–21
Nb + Ta
4.75–5.50
Mo
2.80–3.30
Ti
0.65–1.15
Al
0.20–0.80
Fe
Balance
C
≤0.08
Mn
≤0.35
Si
≤0.35
P
≤0.015
S
≤0.015
B
≤0.006
Cu
≤0.30
Co
≤1.0
Supplied technical reference · Scanned PDF page 4 · printed page 16
Chemical composition

Composition limits · wt.%

Ni
≥58
Cr
20–23
Mo
8–10
Nb + Ta
3.15–4.15
Fe
≤5
C
≤0.10
Mn
≤0.50
Si
≤0.50
P
≤0.015
S
≤0.015
Al
≤0.40
Ti
≤0.40
Co (if determined)
≤1.0
Special Metals · Alloy 625 · Tables 1, 2 & 5; Available Products and Specifications (page 17) ↗
Chemical composition

Composition limits · wt.%

Ni
Balance
Cr
14.5–16.5
Mo
15–17
Fe
4–7
W
3–4.5
Co
≤2.5
C
≤0.01
Mn
≤1.0
P
≤0.04
S
≤0.03
Si
≤0.08
V
≤0.35
Supplied technical reference · Scanned PDF page 6 · printed page 18

Mechanical properties

Reference conditions vary or are incomplete. Read the basis, condition and source for each column; these values do not establish a performance ranking or finished-fastener acceptance values.

Tensile strength1389 MPa
Typical reference sample
Annealed + aged
Room temperature
Special Metals · Alloy 718 · SMC-045, September 2007 · Tables 1 & 8 ↗
724–896 MPa
Nominal reference range
Solution treated
Room temperature
Special Metals · Alloy 625 · Tables 1, 2 & 5; Available Products and Specifications (page 17) ↗
792 MPa
Published reference sample
Mill annealed
Room temperature
Haynes · C-276 · Nominal Composition; Tensile Strength and Elongation; Resistance to Pitting and Crevice Corrosion ↗
0.2% yield strength1207 MPa
Typical reference sample
Annealed + aged
Room temperature
Special Metals · Alloy 718 · SMC-045, September 2007 · Tables 1 & 8 ↗
290–414 MPa
Nominal reference range
Solution treated
Room temperature
Special Metals · Alloy 625 · Tables 1, 2 & 5; Available Products and Specifications (page 17) ↗
356 MPa
Published reference sample
Mill annealed
Room temperature
Haynes · C-276 · Nominal Composition; Tensile Strength and Elongation; Resistance to Pitting and Crevice Corrosion ↗
Elongation20 %
Typical reference sample
Annealed + aged
Room temperature
Special Metals · Alloy 718 · SMC-045, September 2007 · Tables 1 & 8 ↗
40–65 %
Nominal reference range
Solution treated
Room temperature
Special Metals · Alloy 625 · Tables 1, 2 & 5; Available Products and Specifications (page 17) ↗
61 %
Published reference sample
Mill annealed
Room temperature
Haynes · C-276 · Nominal Composition; Tensile Strength and Elongation; Resistance to Pitting and Crevice Corrosion ↗
Reference conditions
Data basis
Typical reference sample
Condition
Annealed + aged
Sample form
Hot-rolled bar · Ø25.4 mm
Sample size
1.0 in diameter (25.4 mm)
Test temperature
Room temperature
Test method
Not documented in this reference
Test direction
Longitudinal
Elongation gauge length
Not documented in this reference
Data basis
Nominal reference range
Condition
Solution treated
Sample form
Rod, bar & plate
Sample size
Up to 101.6 mm
Test temperature
Room temperature
Test method
Not documented in this reference
Test direction
Not documented in this reference
Elongation gauge length
Not documented in this reference
Data basis
Published reference sample
Condition
Mill annealed
Sample form
Sheet · 2 mm thickness
Sample size
0.078 in (2 mm) sheet
Test temperature
Room temperature
Test method
Not documented in this reference
Test direction
Not documented in this reference
Elongation gauge length
Not documented in this reference

Temperature & corrosion

Evaluate the medium, concentration, impurities, temperature and loading together. A melting point or oxidation reference is not a safe working-temperature limit.

Service conditions to reviewSpecify the heat treatment and strength requirement.Match the annealed or solution-treated condition to the application.Check the actual medium, concentration and temperature.
Temperature-dependent data
  • Strength and elongation vs temperaturePlate · mill annealed + aged
View material details
  • Strength and elongation vs temperatureHot-rolled plate · mill annealed at 1052°C
View material details
  • Strength and elongation vs temperatureAnnealed material · supplied reference
View material details

Heat treatment

Delivery condition and heat-treatment requirements are agreed for the requested product form and order.

ConditionAnnealed + agedSolution treatedMill annealed
Reference treatment1750°F / 1 h, then 1325°F / 8 h; furnace cool to 1150°F for 18 h total aging.Special Metals · Alloy 718 · SMC-045, September 2007 · Tables 1 & 8 ↗Not documented in this referenceMill-annealed wrought material context; no heat cycle is attached to this tensile row.Haynes · C-276 · Nominal Composition; Tensile Strength and Elongation; Resistance to Pitting and Crevice Corrosion ↗

Reference applications

Application examples provide context for review; suitability depends on the actual service conditions.

Reference applicationsFasteners · turbine componentsMarine · chemical processingChemical processing · heat exchangers

Standards & documentation

Confirm the edition, product form and condition. Material specifications do not establish finished-fastener compliance.

Material specifications by form
Sources
Sources
Sources
Sources

Documents for your enquiry

Material documentation, EN 10204 3.1, product test reports and third-party inspection can be discussed upon request. The document and inspection scope is agreed at quotation.

Take your shortlist to the next step

Share your drawing or product form, dimensions, quantity and operating conditions. Your selected materials will be included as alternatives for review.

Enquire about selected materials
Request a Quote