Compare Materials: Inconel X-750
MaterialInconel X-750N07750

Summary

Material familyNickel Alloys
Grade / UNSN07750
SummaryAn age-hardenable nickel-chromium alloy used for springs, fasteners and hot-section components.

Performance overview

Material focusStrength developed through aging
Physical referenceNot documented in this reference
Chemical composition
Chemical composition

Selected composition limits · wt.%

Ni + Co
≥70
Cr
14–17
Fe
5–9
Ti
2.25–2.75
Al
0.40–1.00
Nb + Ta
0.70–1.20
Special Metals · X-750 · Table 9 · Ø1/2 in hot-finished bar, treatment B ↗

Mechanical properties

Reference conditions vary or are incomplete. Read the basis, condition and source for each column; these values do not establish a performance ranking or finished-fastener acceptance values.

Tensile strength1351 MPa
Typical reference sample
Solution treated + aged (treatment B)
Room temperature
Special Metals · X-750 · Table 9 · Ø1/2 in hot-finished bar, treatment B ↗
0.2% yield strength1027 MPa
Typical reference sample
Solution treated + aged (treatment B)
Room temperature
Special Metals · X-750 · Table 9 · Ø1/2 in hot-finished bar, treatment B ↗
Elongation24 %
Typical reference sample
Solution treated + aged (treatment B)
Room temperature
Special Metals · X-750 · Table 9 · Ø1/2 in hot-finished bar, treatment B ↗
Reference conditions
Data basis
Typical reference sample
Condition
Solution treated + aged (treatment B)
Sample form
Hot-finished bar
Sample size
Ø12.7 mm (1/2 in)
Test temperature
Room temperature
Test method
Not documented in this reference
Test direction
Not documented in this reference
Elongation gauge length
Not documented in this reference

Temperature & corrosion

Evaluate the medium, concentration, impurities, temperature and loading together. A melting point or oxidation reference is not a safe working-temperature limit.

Service conditions to reviewSpecify the heat treatment; X-750 has several distinct property conditions.
Temperature-dependent dataNot documented in this reference

Heat treatment

Delivery condition and heat-treatment requirements are agreed for the requested product form and order.

ConditionSolution treated + aged (treatment B)
Reference treatment1800°F / 1 h, air cool; 1350°F / 8 h, furnace cool to 1150°F; total aging 18 h.Special Metals · X-750 · Table 9 · Ø1/2 in hot-finished bar, treatment B ↗

Reference applications

Application examples provide context for review; suitability depends on the actual service conditions.

Reference applicationsGas-turbine assemblies · heat-treatment fixtures

Standards & documentation

Confirm the edition, product form and condition. Material specifications do not establish finished-fastener compliance.

Material specifications by form
Sources
Sources

Documents for your enquiry

Every BYBOLT delivery includes an MTC / EN 10204 3.1 certificate, heat-number traceability and mechanical testing. Threaded products include sampled GO / NO-GO gauging. Test methods and acceptance criteria follow the agreed specification; PMI, third-party inspection and additional records are agreed separately at quotation.

Take your shortlist to the next step

Share your drawing or product form, dimensions, quantity and operating conditions. Your selected materials will be included as alternatives for review.

Get a Quote
Get a Quote